How to deal with rust on stainless steel

2007-12-17View Original

Thread Content

Excuse me, gentlemen: the screen frame is made of stainless steel 316L, but the operators used wire brushes for cleaning (which was stopped after it was noticed), and this caused some damage to the surface. After being used for a while, that area started to rust. What should be done in this situation?
Reply #22007-12-17
It can be treated by pickling method, or it can also be processed by polishing method
Reply #32007-12-17
Pickling is used, but the effect is not significant
Reply #42007-12-17
First, use acid cleaning to remove dirt, and then apply electropolishing or mechanical polishing depending on the conditions on site. Polishers are also quite useful these days.
Reply #52007-12-18
Should I polish to remove rust first, and then carry out acid washing and passivation? Is that okay?
Reply #62007-12-20
Pickling is sufficient; there’s no need to polish first, and then passivate it
Reply #72007-12-20
For this carburization process, grinding is usually required first; however, care must be taken to prevent splashing during grinding from causing further carburization, and the depth of grinding should not affect the wall thickness. After grinding, applying pickling paste for passivation is sufficient.
Reply #82007-12-20
The acid wash after dilution will do
Reply #92007-12-21
First, sand it with sandpaper, then pickle and passivate it
Reply #102007-12-21
The rust that forms is due to the wire brush being made of carbon steel. It must be pickled before use.
Reply #112007-12-25
Polishing is sufficient; pickling tends to cause mottling
Reply #122007-12-25
Polishing should work, right? It’s still stainless steel after the rust is removed

Submit a Project

**Looking for Chemical Technology, Equipment & Solutions?** No Registration Required Broader Platform Exposure | Global Chemical Service Provider Connections

Submit Request — Free Consultation

Disclaimer

This is an automated machine translation of the original thread. Some technical terms may have inaccuracies; the original text shall prevail. Click "View Original" at the top right to access the source page, which supports IP-based automatic real-time language translation. Please watch out for contact details and sales inducements to prevent fraud. All content and translations are for reference only, representing solely the poster's personal views. For enquiries, email service@hcbbs.com.