2022-06-13View Original

Thread Content

Can the S22053 material be welded using submerged arc automatic welding? If possible, what welding wire and flux should be used? Has anyone experienced conducting a weld evaluation for the submerged arc welding of 22053?
Reply #22022-06-16
SH∕T 3523-2020 Welding Specifications for Nickel-Containing Stainless Steels, Ferro-Nickel Alloys, Nickel-Based Alloys, and Stainless Steel Composite Steels in the Petrochemical Industry
Reply #32022-06-17
When welding the product, it is important to control the heat input as well as the interlayer temperature, as cracking can occur very easily!
Reply #42022-06-18
It is best not to use automatic welding for S22053, especially for thicker sections, as it tends to crack
Reply #52022-11-19
Submerged arc welding can be used, but it is not recommended; The welding materials are S22053 + SJ601; in addition to routine inspections, microstructural metallographic analysis is also performed to determine the ferrite content.

Submit a Project

**Looking for Chemical Technology, Equipment & Solutions?** No Registration Required Broader Platform Exposure | Global Chemical Service Provider Connections

Submit Request — Free Consultation

Disclaimer

This is an automated machine translation of the original thread. Some technical terms may have inaccuracies; the original text shall prevail. Click "View Original" at the top right to access the source page, which supports IP-based automatic real-time language translation. Please watch out for contact details and sales inducements to prevent fraud. All content and translations are for reference only, representing solely the poster's personal views. For enquiries, email service@hcbbs.com.