For the surfacing of composite plate CS+SS316, is it necessary to test the ferrite content? What is the control range for ferrite content?
Reply #22017-01-17
It is needed. It is generally between 3 and 8. We usually require that the welding materials for the transition layer not be pure austenitic types; they must contain ferrite as well.
Reply #32017-01-18
3-8 are the requirements for welding materials. .
Reply #42017-01-23
For surfacing austenitic materials such as 316, it is not necessary to measure the ferrite content. Double-phase steel needs to be tested.

Submit a Project

**Looking for Chemical Technology, Equipment & Solutions?** No Registration Required Broader Platform Exposure | Global Chemical Service Provider Connections

Submit Request — Free Consultation

Disclaimer

This is an automated machine translation of the original thread. Some technical terms may have inaccuracies; the original text shall prevail. Click "View Original" at the top right to access the source page, which supports IP-based automatic real-time language translation. Please watch out for contact details and sales inducements to prevent fraud. All content and translations are for reference only, representing solely the poster's personal views. For enquiries, email service@hcbbs.com.