The spot welding at the pipe end has penetrated – how should this be dealt with?

2018-07-25View Original

Thread Content

The spot welding at the pipe end has penetrated – how should this be dealt with?
Reply #22018-07-25
Repair or rework strictly in accordance with the welding procedures, based on the equipment requirements and materials
Reply #32018-07-26
Carefully repair the weld using TIG welding, and then grind the inner side
Reply #42018-07-26
This welder definitely hasn’t received any training; change the welder first, and then the pipe!
Reply #52018-07-26
Are there any issues with the welding parameters?
Reply #62018-07-27
Fill it in first, then grind it off with an electric grinder. This situation is encountered quite often.
Reply #72018-07-28
The tube needs to be replaced. The welding heat input is probably too high. Why weld first? Also, looking at the picture, it seems that the length of the heat exchange tubes extending beyond the tube sheet is too large; shouldn’t it be shortened?

Submit a Project

**Looking for Chemical Technology, Equipment & Solutions?** No Registration Required Broader Platform Exposure | Global Chemical Service Provider Connections

Submit Request — Free Consultation

Disclaimer

This is an automated machine translation of the original thread. Some technical terms may have inaccuracies; the original text shall prevail. Click "View Original" at the top right to access the source page, which supports IP-based automatic real-time language translation. Please watch out for contact details and sales inducements to prevent fraud. All content and translations are for reference only, representing solely the poster's personal views. For enquiries, email service@hcbbs.com.